Tc max
21.0 K
Tc ambient
20.0 K
arXiv year
2009
Papers
12
Tc exp.
21.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at single_crystal, resistivity, arXiv:2112.12352, confirmed by 2 papers
Evidence (18 records from 12 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 21.5 | — | polycrystal | resistivity | — | 2013 | T1 | DOI: 10.1103/PhysRevB.88.064502 |
| 21.0 | — | single_crystal | resistivity | — | 2021 | T1 | 2112.12352 |
| 20.0 | — | single_crystal | resistivity, muSR, neutron | — | 2015 | T1 | DOI: 10.1103/PhysRevB.91.024504 |
| 20.0 | — | single_crystal | resistivity | — | 2014 | T1 | 1411.7506 |
| 20.0 | — | single_crystal | — | — | 2010 | T1 | 1009.3941 |
| 19.7 | — | single_crystal | resistivity | — | 2021 | T1 | 2112.12352 |
| 18.5 | — | single_crystal | susceptibility | s-wave | 2010 | T1 | DOI: 10.1103/PhysRevB.81.100501 |
| 18.5 | — | single_crystal | susceptibility | s-wave | 2009 | T1 | 0909.0744 |
| 17.5 | — | single_crystal | resistivity | — | 2021 | T1 | 2112.12352 |
| 17.0 | — | single_crystal | resistivity | s-wave | 2013 | T2 | 1307.1908 |
| 15.0 | — | single_crystal | resistivity, susceptibility | — | 2009 | T1 | 0906.3708 |
| 14.4 | ambient | single_crystal | resistivity | — | 2021 | T1 | 2112.12352 |
| 13.2 | ambient | single_crystal | resistivity | — | 2021 | T1 | 2112.12352 |
| 11.6 | — | single_crystal | resistivity | s-wave | 2013 | T2 | 1307.1908 |
| 10.4 | ambient | single_crystal | resistivity | — | 2021 | T1 | 2112.12352 |
| 8.9 | — | single_crystal | — | — | 2011 | T1 | 1108.2749 |
| — | — | single_crystal | resistivity, microwave | — | 2025 | — | 2504.12049 |
| — | — | single_crystal | — | — | 2018 | T1 | DOI: 10.1103/PhysRevB.97.014511 |
Structure
- Crystal structure
- ThCr2Si2
- Space group
- I4/mmm (#71)
- Lattice a (Å)
- 3.960
- Lattice c (Å)
- 13.020
Superconducting parameters
- Pairing symmetry
- s-wave
- Gap structure
- multi_gap
- λ_eph (e–ph coupling)
- —
Competing orders
- T_SDW
- 82.0 K
- T_AFM
- 40.0 K
Samples & pressure
- Sample form
- single_crystal
- Doping type
- electron
- Doping level
- 0.050