Tc max
37.0 K
Tc ambient
30.0 K
arXiv year
2008
Papers
16
Tc exp.
37.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at single_crystal, susceptibility, arXiv:0902.2522, confirmed by 2 papers
Evidence (17 records from 16 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 38.0 | ambient | single_crystal | resistivity | — | 2008 | T1 | DOI: 10.1103/PhysRevB.78.104527 |
| 37.0 | — | single_crystal | susceptibility | — | 2009 | T2 | 0902.2522 |
| 36.8 | — | single_crystal | resistivity | — | 2011 | T1 | 1101.3150 |
| 32.0 | ambient | single_crystal | susceptibility | — | 2008 | T1 | 0807.4488 |
| 30.0 | — | single_crystal | susceptibility | unknown | 2009 | — | 0902.1804 |
| 30.0 | — | single_crystal | — | — | 2009 | T1 | 0903.0674 |
| 30.0 | — | single_crystal | susceptibility | — | 2009 | T1 | DOI: 10.1103/PhysRevB.80.020501 |
| 30.0 | — | single_crystal | resistivity | s-wave | 2009 | T1 | DOI: 10.1103/PhysRevB.79.012503 |
| 30.0 | ambient | — | resistivity | — | 2008 | — | 0810.0241 |
| 30.0 | — | single_crystal | muSR | s-wave | 2008 | T1 | DOI: 10.1103/PhysRevB.78.214503 |
| 30.0 | — | single_crystal | resistivity, susceptibility, specific_heat | — | 2008 | T1 | 0806.1874 |
| 30.0 | — | single_crystal | muSR | — | 2008 | T1 | 0807.1044 |
| 28.0 | — | single_crystal | resistivity | — | 2009 | T1 | DOI: 10.1103/PhysRevLett.102.187003 |
| 27.0 | — | single_crystal | resistivity | s-wave | 2009 | T1 | DOI: 10.1103/PhysRevB.79.012503 |
| 27.0 | — | single_crystal | resistivity | s-wave | 2008 | T1 | 0809.1566 |
| — | — | — | resistivity | — | 2008 | T1 | 0809.1080 |
| — | — | single_crystal | resistivity | — | 2008 | — | 0807.1089 |
Structure
- Crystal structure
- ThCr2Si2-type
- Space group
- I4/mmm
- Lattice a (Å)
- 3.930
- Lattice c (Å)
- 13.130
Superconducting parameters
- Pairing symmetry
- s-wave
- Gap structure
- multi_gap
- Hc2
- 130.0 T (0 K, estimated from scaling behavior)
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Sample form
- single_crystal
- Doping type
- hole
- Doping level
- 0.450