Tc max
92.2 K
Tc ambient
91.0 K
arXiv year
1990
Papers
30
Tc exp.
92.2 K
Tc theo.
—
Evidence
experimental
Tc max measured at single_crystal, resistivity, arXiv:cond-mat/0009476, confirmed by 3 papers
Evidence (46 records from 30 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 94.0 | — | single_crystal | susceptibility | — | 1998 | T1 | DOI: 10.1103/PhysRevB.57.10946 |
| 92.2 | — | single_crystal | resistivity | — | 2000 | T1 | cond-mat/0009476 |
| 92.2 | — | single_crystal | resistivity | — | 2000 | T1 | DOI: 10.1103/PhysRevLett.85.3716 |
| 92.0 | — | polycrystal | susceptibility | — | 1991 | T1 | DOI: 10.1103/PhysRevB.43.10445 |
| 91.0 | — | single_crystal | resistivity | — | 1998 | T1 | cond-mat/9812354 |
| 90.0 | — | single_crystal | resistivity | — | 1992 | T1 | DOI: 10.1103/PhysRevB.46.14234 |
| 89.0 | — | — | resistivity | — | 2001 | T3 | cond-mat/0111128 |
| 89.0 | — | single_crystal | susceptibility | — | 1996 | T1 | DOI: 10.1103/PhysRevB.53.R14749 |
| 89.0 | — | polycrystal | resistivity | — | 1990 | T1 | DOI: 10.1103/PhysRevB.41.6679 |
| 88.0 | — | single_crystal | susceptibility | — | 1998 | T1 | DOI: 10.1103/PhysRevB.57.10946 |
| 88.0 | — | single_crystal | susceptibility | — | 1994 | T1 | DOI: 10.1103/PhysRevB.49.1315 |
| 87.0 | — | — | resistivity | — | 2001 | T3 | cond-mat/0111128 |
| 86.0 | — | single_crystal | susceptibility | — | 2010 | T1 | DOI: 10.1103/PhysRevB.81.214520 |
| 86.0 | — | single_crystal | resistivity | d-wave | 2000 | T1 | DOI: 10.1103/PhysRevB.61.3616 |
| 86.0 | — | single_crystal | susceptibility | — | 1994 | T1 | DOI: 10.1103/PhysRevB.49.1315 |
| 85.0 | — | single_crystal | — | — | 2008 | T1 | 0808.3896 |
| 84.0 | ambient | single_crystal | resistivity | — | 2009 | T1 | DOI: 10.1103/PhysRevB.79.134505 |
| 84.0 | — | single_crystal | susceptibility | — | 1998 | T1 | DOI: 10.1103/PhysRevB.58.R8929 |
| 84.0 | — | single_crystal | susceptibility | — | 1997 | T1 | DOI: 10.1103/PhysRevLett.78.3177 |
| 83.5 | — | single_crystal | resistivity | — | 2000 | T1 | DOI: 10.1103/PhysRevB.62.11384 |
| 83.0 | — | polycrystal | resistivity | — | 1990 | T1 | DOI: 10.1103/PhysRevB.41.6679 |
| 82.0 | — | — | resistivity | — | 2001 | T3 | cond-mat/0111128 |
| 81.0 | — | single_crystal | susceptibility | — | 1997 | T1 | DOI: 10.1103/PhysRevLett.78.3177 |
| 80.0 | — | polycrystal | resistivity | — | 1991 | T1 | DOI: 10.1103/PhysRevB.43.12976 |
| 78.0 | ambient | polycrystal | resistivity | — | 1992 | T1 | DOI: 10.1103/PhysRevB.46.5686 |
| 77.0 | — | single_crystal | susceptibility | — | 1997 | T1 | DOI: 10.1103/PhysRevLett.78.3177 |
| 75.0 | — | thin_film | resistivity | d-wave | 2000 | T1 | DOI: 10.1103/PhysRevB.61.689 |
| 75.0 | — | single_crystal | — | — | 1995 | T1 | DOI: 10.1103/PhysRevB.52.82 |
| 75.0 | — | polycrystal | resistivity | — | 1990 | T1 | DOI: 10.1103/PhysRevB.41.6679 |
| 74.0 | ambient | single_crystal | resistivity | — | 2009 | T1 | DOI: 10.1103/PhysRevB.79.134505 |
| 74.0 | — | polycrystal | susceptibility | — | 1995 | T1 | DOI: 10.1103/PhysRevB.51.9352 |
| 70.0 | ambient | single_crystal | resistivity | — | 2009 | T1 | DOI: 10.1103/PhysRevB.79.134505 |
| 68.0 | — | thin_film | resistivity | d-wave | 2002 | T1 | DOI: 10.1103/PhysRevLett.89.017005 |
| 67.0 | — | thin_film | resistivity | d-wave | 2002 | T1 | DOI: 10.1103/PhysRevLett.89.017005 |
| 67.0 | — | polycrystal | — | — | 1995 | T1 | DOI: 10.1103/PhysRevB.52.82 |
| 67.0 | — | single_crystal | resistivity | — | 1992 | T1 | DOI: 10.1103/PhysRevB.46.5773 |
| 65.0 | — | single_crystal | STM | — | 2002 | T3 | cond-mat/0202450 |
| 65.0 | — | polycrystal | susceptibility | — | 1991 | T1 | DOI: 10.1103/PhysRevB.43.10445 |
| 63.0 | — | thin_film | resistivity | d-wave | 2002 | T1 | DOI: 10.1103/PhysRevLett.89.017005 |
| 50.0 | ambient | single_crystal | resistivity | — | 2009 | T1 | DOI: 10.1103/PhysRevB.79.134505 |
| 43.0 | ambient | single_crystal | resistivity | — | 2009 | T1 | DOI: 10.1103/PhysRevB.79.134505 |
| — | — | single_crystal | resistivity | — | 2021 | T1 | DOI: 10.1103/PhysRevB.104.L020503 |
| — | — | polycrystal | susceptibility | — | 2002 | T1 | DOI: 10.1103/PhysRevB.66.224510 |
| — | — | — | resistivity | — | 1999 | T1 | cond-mat/9908190 |
| — | — | single_crystal | susceptibility | — | 1997 | T1 | DOI: 10.1103/PhysRevB.55.14479 |
| — | — | single_crystal | susceptibility | — | 1990 | T1 | DOI: 10.1103/PhysRevB.42.412 |
Structure
- Crystal structure
- orthorhombic
- Lattice a (Å)
- 5.410
- Lattice c (Å)
- 30.680
Superconducting parameters
- Pairing symmetry
- d-wave
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Sample form
- single_crystal
- Substrate
- SrTiO3
- Pressure type
- none
- Doping type
- hole