Tc max
10.0 K
Tc ambient
8.6 K
arXiv year
2012
Papers
16
Tc exp.
10.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at polycrystal, resistivity, arXiv:1207.4955, confirmed by 2 papers
Evidence (30 records from 16 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 14.0 | ambient | polycrystal | STM | — | 2013 | T1 | 1304.3354 |
| 10.0 | — | polycrystal | resistivity | — | 2012 | T1 | 1207.4955 |
| 8.6 | — | polycrystal | resistivity | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.220510 |
| 6.2 | ambient | polycrystal | resistivity | — | 2013 | T1 | 1304.3354 |
| 6.0 | — | polycrystal | susceptibility | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.220510 |
| 5.3 | — | polycrystal | susceptibility | s-wave | 2013 | T1 | 1304.4386 |
| 5.0 | — | — | susceptibility | s-wave | 2013 | T1 | 1305.6913 |
| 4.8 | — | polycrystal | resistivity | s-wave | 2013 | T1 | DOI: 10.1103/PhysRevB.88.224515 |
| 4.8 | — | — | — | — | 2013 | T1 | 1307.0645 |
| 4.8 | ambient | polycrystal | resistivity | s-wave | 2013 | T1 | 1309.7282 |
| 4.6 | — | polycrystal | resistivity | s-wave | 2013 | T1 | DOI: 10.1103/PhysRevB.88.224515 |
| 4.6 | ambient | polycrystal | resistivity, muSR | s-wave | 2013 | T1 | 1309.7282 |
| 4.6 | — | polycrystal | resistivity | — | 2012 | T1 | 1207.4955 |
| 4.5 | — | polycrystal | muSR | s-wave | 2013 | T1 | DOI: 10.1103/PhysRevB.88.224515 |
| 4.5 | — | polycrystal | resistivity, susceptibility | — | 2013 | T1 | 1311.0161 |
| 4.5 | — | polycrystal | resistivity | — | 2012 | T1 | 1207.5395 |
| 4.5 | — | polycrystal | resistivity | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.220510 |
| 4.4 | — | polycrystal | susceptibility, resistivity | — | 2012 | T1 | 1207.5428 |
| 4.4 | — | polycrystal | specific_heat | — | 2012 | T1 | 1208.2796 |
| 4.3 | — | — | — | — | 2013 | T1 | 1307.0645 |
| 4.2 | ambient | polycrystal | resistivity | — | 2013 | T1 | 1304.3354 |
| 4.1 | — | polycrystal | resistivity | — | 2012 | T1 | 1207.5395 |
| 4.0 | — | polycrystal | susceptibility | — | 2012 | T1 | 1207.5395 |
| 3.7 | ambient | polycrystal | resistivity | — | 2013 | T1 | 1304.3354 |
| 3.6 | ambient | polycrystal | susceptibility | — | 2013 | T1 | 1304.3354 |
| 3.6 | — | polycrystal | susceptibility | — | 2012 | T1 | 1207.4955 |
| — | — | — | — | — | 2024 | — | 2405.09129 |
| — | — | polycrystal | resistivity, susceptibility | unknown | 2020 | T1 | 2007.06696 |
| — | — | polycrystal | resistivity, susceptibility | — | 2012 | — | 1208.5307 |
| — | — | — | resistivity | — | 2012 | T1 | 1207.6935 |
Structure
- Crystal structure
- layered
- Space group
- I4/mmm
- Lattice a (Å)
- 3.970
- Lattice c (Å)
- 41.352
Superconducting parameters
- Pairing symmetry
- s-wave
- Gap structure
- multi_gap
- Hc2
- 31.0 T (0 K)
- λ_eph (e–ph coupling)
- —
Competing orders
- ρ(T) exponent
- 2.00
Samples & pressure
- Sample form
- polycrystal
- Pressure type
- none
- Doping type
- none