Tc max
8.9 K
Tc ambient
7.5 K
arXiv year
2011
Papers
17
Tc exp.
8.9 K
Tc theo.
—
Evidence
experimental
Tc max measured at P=4 GPa, single_crystal, susceptibility, DOI: 10.1103/PhysRevLett.109.237008, confirmed by 2 papers
Evidence (25 records from 17 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 8.9 | 4.0 | single_crystal | susceptibility | — | 2012 | T1 | DOI: 10.1103/PhysRevLett.109.237008 |
| 8.9 | 4.0 | single_crystal | susceptibility | — | 2011 | T2 | 1105.3941 |
| 7.5 | — | single_crystal | resistivity | — | 2016 | T1 | 1604.08948 |
| 7.5 | — | single_crystal | resistivity | s-wave | 2012 | T1 | DOI: 10.1103/PhysRevB.86.024522 |
| 7.3 | — | single_crystal | resistivity | s-wave | 2012 | T1 | DOI: 10.1103/PhysRevB.86.064504 |
| 7.3 | — | single_crystal | resistivity | — | 2012 | T1 | 1202.5164 |
| 7.1 | — | single_crystal | susceptibility | — | 2024 | T1 | 2403.14891 |
| 7.1 | — | single_crystal | susceptibility | — | 2014 | T1 | 1408.1525 |
| 7.0 | ambient | single_crystal | resistivity, susceptibility | — | 2023 | T3 | 2308.08679 |
| 7.0 | — | single_crystal | resistivity | s-wave | 2016 | T1 | DOI: 10.1103/PhysRevB.93.134505 |
| 7.0 | — | single_crystal | susceptibility | — | 2016 | T1 | 1604.08948 |
| 7.0 | — | single_crystal | susceptibility, specific_heat | s-wave | 2012 | T1 | DOI: 10.1103/PhysRevB.86.024522 |
| 7.0 | — | single_crystal | susceptibility | — | 2024 | T1 | 2403.14891 |
| 6.9 | — | single_crystal | susceptibility | s-wave | 2012 | T1 | DOI: 10.1103/PhysRevB.86.064504 |
| 6.9 | — | single_crystal | susceptibility | — | 2012 | T1 | 1202.5164 |
| 6.8 | — | single_crystal | specific_heat | s-wave | 2016 | T1 | DOI: 10.1103/PhysRevB.93.134505 |
| 6.8 | — | single_crystal | susceptibility, muSR | — | 2013 | T1 | DOI: 10.1103/PhysRevB.88.104505 |
| 6.8 | ambient | single_crystal | muSR | s-wave | 2015 | T1 | DOI: 10.1103/PhysRevB.92.195122 |
| 6.4 | ambient | single_crystal | susceptibility | — | 2011 | T2 | 1105.3941 |
| 4.5 | — | polycrystal | NMR | s-wave | 2014 | — | 1406.3544 |
| — | — | — | resistivity | — | 2021 | T1 | 2110.02025 |
| — | — | — | — | s-wave | 2018 | — | 1805.02820 |
| — | — | — | muSR | s-wave | 2015 | T1 | 1506.04995 |
| — | — | single_crystal | muSR | s-wave | 2013 | T1 | 1305.0844 |
| — | — | single_crystal | resistivity | — | 2012 | T1 | 1202.5164 |
Structure
- Crystal structure
- Pm3̄n
- Space group
- Pm3̄n
- Phase
- infinite_layer
- Lattice a (Å)
- 9.708
- Lattice c (Å)
- 9.708
Superconducting parameters
- Pairing symmetry
- s-wave
- Gap structure
- full_gap
- Hc2
- 7.0 T (at T=2 K)
- λ_eph (e–ph coupling)
- —
Competing orders
- Competing order
- CDW
- T_CDW
- 40.0 K
- ρ(T) exponent
- 2.00
Samples & pressure
- Sample form
- single_crystal
- Doping type
- none
- Doping level
- 0.000