Tc max
8.6 K
Tc ambient
0.4 K
arXiv year
2014
Papers
4
Tc exp.
8.6 K
Tc theo.
—
Evidence
experimental
Tc max measured at P=1.4 GPa, polycrystal, resistivity, DOI: 10.1103/PhysRevB.91.214512, confirmed by 4 papers
Evidence (12 records from 4 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 8.6 | 1.4 | polycrystal | resistivity | — | 2015 | T1 | DOI: 10.1103/PhysRevB.91.214512 |
| 8.6 | 1.5 | polycrystal | susceptibility | — | 2015 | T1 | DOI: 10.1103/PhysRevB.91.214512 |
| 8.6 | 1.7 | polycrystal | resistivity | — | 2015 | T1 | 1505.04704 |
| 8.6 | 1.5 | polycrystal | susceptibility | — | 2015 | T1 | 1505.04704 |
| 0.7 | 1.1 | polycrystal | susceptibility | — | 2015 | T1 | DOI: 10.1103/PhysRevB.91.214512 |
| 0.7 | 1.1 | polycrystal | susceptibility | — | 2015 | T1 | 1505.04704 |
| 0.4 | 0.4 | polycrystal | susceptibility | — | 2015 | T1 | DOI: 10.1103/PhysRevB.91.214512 |
| 0.4 | 0.4 | polycrystal | susceptibility | — | 2015 | T1 | 1505.04704 |
| 0.3 | ambient | polycrystal | resistivity | — | 2015 | T1 | DOI: 10.1103/PhysRevB.91.214512 |
| 0.3 | ambient | polycrystal | resistivity | — | 2015 | T1 | 1505.04704 |
| 0.3 | ambient | polycrystal | resistivity | — | 2014 | T1 | 1407.7132 |
| 0.3 | ambient | polycrystal | resistivity | — | 2014 | T1 | DOI: 10.1103/PhysRevB.90.064518 |
Structure
- Crystal structure
- CeBiS2O-type
- Space group
- P4/nmm (No. 129)
- Lattice a (Å)
- 4.051
- Lattice c (Å)
- 13.534
Superconducting parameters
- Hc2
- 0.2 T (0.018 K)
- λ_eph (e–ph coupling)
- —
Competing orders
- Competing order
- CDW
- T_CDW
- 280.0 K
Samples & pressure
- Sample form
- polycrystal
- Pressure type
- hydrostatic