Tc max
36.9 K
Tc ambient
36.9 K
arXiv year
2018
Papers
11
Tc exp.
36.9 K
Tc theo.
—
Evidence
experimental
Tc max measured at ambient, single_crystal, resistivity, arXiv:2108.03184, confirmed by 2 papers
Evidence (17 records from 11 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 37.0 | — | — | — | — | 2023 | T1 | 2306.16570 |
| 36.9 | ambient | single_crystal | resistivity | — | 2021 | T1 | 2108.03184 |
| 36.6 | ambient | single_crystal | resistivity | — | 2019 | T1 | DOI: 10.1103/PhysRevB.99.144509 |
| 36.5 | — | single_crystal | susceptibility, resistivity | — | 2021 | T1 | DOI: 10.1103/PhysRevB.103.195112 |
| 36.5 | — | single_crystal | resistivity, susceptibility | s_pm | 2020 | T1 | 2010.02110 |
| 36.5 | — | polycrystal | susceptibility | s_pm | 2019 | T1 | 1907.03839 |
| 36.3 | — | single_crystal | resistivity, susceptibility | — | 2018 | — | 1807.04135 |
| 36.3 | — | single_crystal | resistivity | s-wave | 2018 | T1 | DOI: 10.1103/PhysRevB.98.140506 |
| 36.0 | — | single_crystal | susceptibility | s-wave | 2018 | T1 | DOI: 10.1103/PhysRevB.98.140506 |
| 35.3 | ambient | single_crystal | resistivity | — | 2021 | T1 | 2108.03184 |
| 35.0 | ambient | single_crystal | resistivity | — | 2019 | T1 | 1902.08667 |
| 35.0 | ambient | single_crystal | susceptibility | — | 2019 | T1 | DOI: 10.1103/PhysRevB.99.144509 |
| 34.8 | — | single_crystal | susceptibility | — | 2019 | T1 | 1906.04597 |
| 27.1 | ambient | single_crystal | resistivity | — | 2021 | T1 | 2108.03184 |
| 23.5 | 6.2 | single_crystal | resistivity | — | 2019 | T1 | DOI: 10.1103/PhysRevB.99.144509 |
| — | — | — | — | — | 2021 | T1 | 2110.09675 |
| — | — | single_crystal | resistivity, susceptibility | — | 2019 | T1 | 1902.08667 |
Structure
- Crystal structure
- tetragonal
- Space group
- P4/mmm
- Lattice a (Å)
- 3.859
- Lattice c (Å)
- 13.186
Superconducting parameters
- Gap structure
- multi_gap
- λ_eph (e–ph coupling)
- —
Competing orders
- T_AFM
- 15.0 K
Samples & pressure
- Sample form
- single_crystal
- Pressure type
- hydrostatic