Tc max
79.0 K
Tc ambient
79.0 K
arXiv year
1989
Papers
2
Tc exp.
79.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at polycrystal, susceptibility, DOI: 10.1103/PhysRevLett.84.1990, confirmed by 2 papers
Evidence (3 records from 2 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 79.0 | — | polycrystal | susceptibility | — | 2000 | T1 | DOI: 10.1103/PhysRevLett.84.1990 |
| 78.5 | — | polycrystal | susceptibility | — | 2000 | T1 | DOI: 10.1103/PhysRevLett.84.1990 |
| 77.4 | — | polycrystal | susceptibility | — | 1989 | T1 | DOI: 10.1103/PhysRevB.39.7347 |
Structure
- Crystal structure
- Ammm
- Space group
- Ammm
- Lattice a (Å)
- 3.840
- Lattice c (Å)
- 27.221
Superconducting parameters
- Pairing symmetry
- d-wave
- λ_eph (e–ph coupling)
- —
Competing orders
- T_CDW
- 220.0 K
Samples & pressure
- Sample form
- polycrystal