Tc max
15.2 K
Tc ambient
—
arXiv year
2003
Papers
11
Tc exp.
15.2 K
Tc theo.
4.3 K
Evidence
experimental
Tc max measured at powder, susceptibility, DOI: 10.1103/PhysRevLett.97.107001, confirmed by 2 papers
Evidence (18 records from 11 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 15.4 | — | single_crystal | resistivity | — | 2018 | T1 | DOI: 10.1103/PhysRevB.98.064512 |
| 15.2 | — | powder | susceptibility | — | 2006 | T1 | DOI: 10.1103/PhysRevLett.97.107001 |
| 15.1 | — | polycrystal | susceptibility | — | 2010 | T1 | DOI: 10.1103/PhysRevB.81.014525 |
| 15.0 | — | polycrystal | susceptibility | — | 2010 | T1 | DOI: 10.1103/PhysRevB.82.054504 |
| 14.0 | — | polycrystal | susceptibility | — | 2010 | T1 | DOI: 10.1103/PhysRevB.81.014525 |
| 14.0 | — | polycrystal | specific_heat | — | 2009 | T1 | DOI: 10.1103/PhysRevLett.103.077004 |
| 12.6 | — | polycrystal | susceptibility | — | 2010 | T1 | DOI: 10.1103/PhysRevB.81.014525 |
| 12.5 | — | polycrystal | susceptibility, muSR | — | 2010 | T1 | DOI: 10.1103/PhysRevB.81.014525 |
| 12.2 | — | polycrystal | susceptibility | — | 2010 | T1 | DOI: 10.1103/PhysRevB.82.054504 |
| 11.6 | — | polycrystal | susceptibility, muSR | — | 2010 | T1 | DOI: 10.1103/PhysRevB.81.014525 |
| 11.6 | — | polycrystal | specific_heat | — | 2009 | T1 | DOI: 10.1103/PhysRevLett.103.077004 |
| 11.5 | — | single_crystal | resistivity | — | 2018 | T1 | DOI: 10.1103/PhysRevB.98.064512 |
| 11.0 | — | polycrystal | susceptibility | s-wave | 2014 | T1 | DOI: 10.1103/PhysRevB.90.020503 |
| 4.3 | — | — | — | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.054513 |
| — | — | — | — | — | 2024 | T1 | 2403.03025 |
| — | — | single_crystalline | resistivity | — | 2018 | T1 | 1808.06635 |
| — | — | — | — | unknown | 2014 | T1 | 1407.3031 |
| — | — | — | muSR, magnetization | — | 2003 | T1 | cond-mat/0310736 |
Structure
- Crystal structure
- beta-ZrNCl
Superconducting parameters
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Sample form
- polycrystal
- Doping type
- electron
- Doping level
- 0.110