Tc max
38.6 K
Tc ambient
38.6 K
arXiv year
2003
Papers
7
Tc exp.
38.6 K
Tc theo.
—
Evidence
experimental
Tc max measured at wire, resistivity, DOI: 10.1103/PhysRevLett.92.217003, confirmed by 4 papers
Evidence (11 records from 7 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 38.6 | — | wire | resistivity | — | 2004 | T1 | DOI: 10.1103/PhysRevLett.92.217003 |
| 37.9 | — | wire | resistivity | — | 2004 | T1 | DOI: 10.1103/PhysRevLett.92.217003 |
| 36.2 | — | wire | resistivity, susceptibility | — | 2004 | T1 | DOI: 10.1103/PhysRevLett.92.217003 |
| 35.4 | — | single_crystal | susceptibility | — | 2006 | T1 | DOI: 10.1103/PhysRevB.74.144511 |
| 33.1 | — | single_crystal | susceptibility | — | 2006 | T1 | DOI: 10.1103/PhysRevB.74.144511 |
| 30.6 | — | single_crystal | susceptibility | — | 2006 | T1 | DOI: 10.1103/PhysRevB.74.144511 |
| 19.0 | — | single_crystal | resistivity | — | 2005 | T1 | DOI: 10.1103/PhysRevB.71.060503 |
| 9.0 | — | single_crystal | — | — | 2003 | T1 | cond-mat/0304656 |
| — | — | polycrystal | ARPES | — | 2005 | T1 | DOI: 10.1103/PhysRevB.72.064527 |
| — | — | — | — | — | 2004 | T1 | cond-mat/0409219 |
| — | — | single_crystal | resistivity, susceptibility | — | 2003 | T1 | cond-mat/0305485 |
Superconducting parameters
- Gap structure
- multi_gap
- Hc2
- 32.0 T (0 K)
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Doping level
- 0.038