Tc max
27.0 K
Tc ambient
27.0 K
arXiv year
2012
Papers
16
Tc exp.
27.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at single_crystal, susceptibility, arXiv:1201.2966, confirmed by 2 papers
Evidence (20 records from 16 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 31.0 | — | single_crystal | resistivity, susceptibility | — | 2012 | T2 | 1207.5382 |
| 27.0 | — | single_crystal | susceptibility | — | 2012 | T1 | 1201.2966 |
| 21.2 | — | single_crystal | susceptibility | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.214512 |
| 20.0 | — | single_crystal | STM | — | 2012 | T1 | DOI: 10.1103/PhysRevLett.109.037002 |
| 16.8 | — | single_crystal | susceptibility | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.214512 |
| 16.0 | ambient | single_crystal | neutron | s_pm | 2018 | — | 1807.09669 |
| 16.0 | — | single_crystal | resistivity | — | 2018 | T1 | DOI: 10.1103/PhysRevB.97.020505 |
| 14.0 | — | single_crystal | neutron | s_pm | 2018 | — | 1807.09669 |
| 14.0 | — | single_crystal | susceptibility | — | 2012 | T1 | 1201.2966 |
| 13.0 | — | single_crystal | STM | — | 2012 | T1 | DOI: 10.1103/PhysRevLett.109.037002 |
| 10.0 | — | — | muSR | — | 2014 | T1 | 1406.2412 |
| 6.0 | — | single_crystal | resistivity | — | 2012 | T1 | DOI: 10.1103/PhysRevB.86.155143 |
| — | — | single_crystal | susceptibility, resistivity | — | 2018 | T1 | 1810.08777 |
| — | — | — | susceptibility, muSR | — | 2016 | T1 | 1112.0419 |
| — | — | — | — | d-wave | 2014 | T1 | 1410.6456 |
| — | — | single_crystal | ARPES | — | 2014 | T1 | DOI: 10.1103/PhysRevX.4.031041 |
| — | — | — | resistivity, susceptibility | s_pm | 2013 | T1 | 1312.3171 |
| — | — | single_crystal | specific_heat | — | 2013 | T1 | DOI: 10.1103/PhysRevB.87.144512 |
| — | — | polycrystal | susceptibility, muSR | — | 2012 | T1 | DOI: 10.1103/PhysRevB.85.054503 |
| — | — | single_crystal | specific_heat | s-wave | 2012 | T1 | 1211.5844 |
Structure
- Crystal structure
- orthorhombic
- Lattice a (Å)
- 5.570
- Lattice c (Å)
- 6.970
Superconducting parameters
- Pairing symmetry
- s_pm
- Hc2
- 40.0 T (underdoped)
- λ_eph (e–ph coupling)
- —
Competing orders
- Competing order
- AFM
- T_AFM
- 28.0 K
- ρ(T) exponent
- 1.00
Samples & pressure
- Sample form
- single_crystal
- Pressure type
- none
- Doping type
- electron
- Doping level
- 0.032