← Materials
Nd_1.85Ce_0.15CuO_4
cuprate · T' tetragonal
ambient SCunconventional2D / interfacecompeting orderdisputed
Tc max
25.0 K
Tc ambient
25.0 K
Discovery
1996
Papers
35
Tc max measured at ambient, single_crystal, resistivity, arXiv:cond-mat/0103480, confirmed by 4 papers
Evidence (41 records from 35 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Paper |
|---|---|---|---|---|---|---|
| 25.0 | ambient | single_crystal | — | — | 2004 | cond-mat/0403258 |
| 25.0 | ambient | single_crystal | neutron | d-wave | 2004 | cond-mat/0410250 |
| 25.0 | ambient | single_crystal | resistivity | — | 2001 | cond-mat/0103480 |
| 25.0 | ambient | single_crystal | susceptibility | d-wave | 2001 | cond-mat/0107244 |
| 24.0 | ambient | single_crystal | resistivity, susceptibility | — | 2002 | cond-mat/0212172 |
| 24.0 | ambient | thin_film | STM, resistivity | — | 2001 | cond-mat/0101433 |
| 24.0 | ambient | single_crystal | susceptibility | d-wave | 2001 | cond-mat/0107244 |
| 24.0 | ambient | thin_film | resistivity | s-wave | 1998 | cond-mat/9805162 |
| 23.5 | ambient | thin_film | resistivity | — | 2002 | cond-mat/0205090 |
| 23.5 | ambient | thin_film | resistivity | — | 2000 | cond-mat/0002341 |
| 23.0 | ambient | — | — | — | 2004 | cond-mat/0405016 |
| 23.0 | ambient | — | — | — | 1997 | cond-mat/9711194 |
| 22.5 | ambient | thin_film | resistivity | — | 2002 | cond-mat/0205090 |
| 22.0 | ambient | single_crystal | — | d-wave | 2005 | cond-mat/0501621 |
| 22.0 | ambient | single_crystal | susceptibility | d-wave | 2003 | cond-mat/0304175 |
| 22.0 | ambient | single_crystal | susceptibility | — | 2002 | cond-mat/0201538 |
| 21.0 | ambient | thin_film | susceptibility | — | 2004 | cond-mat/0408100 |
| 21.0 | ambient | — | susceptibility | s-wave | 2004 | cond-mat/0408105 |
| 20.1 | ambient | thin_film | susceptibility | d-wave | 2000 | cond-mat/0003404 |
| 20.1 | ambient | thin_film | susceptibility, resistivity | d-wave | 2000 | cond-mat/0005515 |
| 20.0 | ambient | thin_film | resistivity | d-wave | 2005 | cond-mat/0503429 |
| 18.0 | ambient | single_crystal | — | — | 2004 | cond-mat/0403258 |
| 16.9 | ambient | thin_film | susceptibility, resistivity | d-wave | 2000 | cond-mat/0005515 |
| 12.5 | ambient | thin_film | resistivity | — | 2002 | cond-mat/0205090 |
| — | — | — | STM | — | 2004 | cond-mat/0405073 |
| — | ambient | — | resistivity | — | 2004 | cond-mat/0406340 |
| — | ambient | — | resistivity | d-wave | 2004 | cond-mat/0411069 |
| — | ambient | — | — | — | 2003 | cond-mat/0307454 |
| — | ambient | — | susceptibility | — | 2003 | cond-mat/0308236 |
| — | ambient | single_crystal | neutron | — | 2003 | cond-mat/0310289 |
| — | ambient | single_crystal | susceptibility | — | 2002 | cond-mat/0201024 |
| — | ambient | — | susceptibility | s-wave | 2001 | cond-mat/0112401 |
| — | ambient | single_crystal | STM | unknown | 2000 | cond-mat/0002141 |
| — | ambient | single_crystal | susceptibility | s-wave | 2000 | cond-mat/0002301 |
| — | ambient | thin_film | — | d-wave | 2000 | cond-mat/0002341 |
| — | ambient | thin_film | — | d-wave | 2000 | cond-mat/0004185 |
| — | ambient | single_crystal | ARPES | d-wave | 2000 | cond-mat/0012003 |
| — | ambient | single_crystal | susceptibility | d-wave | 1999 | cond-mat/9912001 |
| — | ambient | — | — | — | 1998 | cond-mat/9806064 |
| — | ambient | thin_film | STM | s-wave | 1998 | cond-mat/9806150 |
| — | ambient | — | — | — | 1996 | cond-mat/9610050 |
Structure
- Crystal structure
- T' tetragonal
- Space group
- I4/mmm (#139)
- Lattice a (Å)
- 3.950
- Lattice c (Å)
- 12.070
Superconducting parameters
- Pairing symmetry
- d-wave
- Gap structure
- nodal
- Hc2
- 8.0 T (2.2 K, H parallel c)
- λ_eph (e–ph coupling)
- —
Competing orders
- Competing order
- AFM
- T_AFM
- 220.0 K
- ρ(T) exponent
- 2.00
Samples & pressure
- Substrate
- SrTiO_3
- Pressure type
- none
- Doping type
- electron
- Doping level
- 0.150