RuSr2(Gd1.5Ce0.5)Cu2O10-δ
cuprate · tetragonal · 1222
ambient SCunconventionalcompeting orderdisputed
Tc max
45.0 K
Tc ambient
45.0 K
arXiv year
2001
Papers
13
Tc exp.
45.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at ambient, polycrystal, resistivity, arXiv:cond-mat/0511718, confirmed by 3 papers
Evidence (34 records from 13 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 59.0 | — | polycrystal | — | — | 2005 | T2 | cond-mat/0511489 |
| 58.0 | — | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 45.0 | ambient | polycrystal | resistivity | — | 2005 | T1 | cond-mat/0511718 |
| 45.0 | — | polycrystal | susceptibility | — | 2002 | T2 | cond-mat/0209593 |
| 44.0 | — | polycrystal | — | — | 2005 | T2 | cond-mat/0511489 |
| 43.0 | — | — | resistivity | — | 2002 | T1 | cond-mat/0211644 |
| 42.9 | — | polycrystal | susceptibility | — | 2005 | T1 | DOI: 10.1103/PhysRevB.71.134509 |
| 41.5 | — | polycrystal | — | — | 2005 | T2 | cond-mat/0511489 |
| 40.0 | ambient | polycrystal | susceptibility | — | 2005 | T2 | cond-mat/0511489 |
| 40.0 | — | polycrystal | resistivity | — | 2002 | T2 | cond-mat/0209593 |
| 40.0 | — | — | susceptibility | — | 2002 | T1 | cond-mat/0211644 |
| 39.0 | ambient | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 37.5 | — | polycrystal | specific_heat | — | 2009 | — | 0910.2384 |
| 37.5 | — | polycrystal | specific_heat | — | 2005 | T2 | cond-mat/0511489 |
| 37.5 | ambient | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 37.0 | ambient | polycrystal | specific_heat | — | 2005 | T2 | cond-mat/0511489 |
| 37.0 | — | polycrystal | specific_heat | — | 2005 | T2 | cond-mat/0511489 |
| 35.0 | ambient | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 35.0 | — | polycrystal | resistivity | — | 2004 | T1 | DOI: 10.1103/PhysRevB.70.104520 |
| 34.7 | — | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 32.8 | ambient | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 32.5 | — | polycrystal | resistivity | — | 2003 | T1 | DOI: 10.1103/PhysRevB.68.144512 |
| 32.0 | — | polycrystal | resistivity | — | 2004 | T1 | cond-mat/0403229 |
| 25.0 | — | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 22.8 | — | polycrystal | — | — | 2005 | T2 | cond-mat/0511489 |
| 22.0 | — | polycrystal | susceptibility | — | 2005 | T1 | DOI: 10.1103/PhysRevB.71.064520 |
| 22.0 | — | polycrystal | susceptibility | — | 2004 | T2 | cond-mat/0410396 |
| 18.5 | ambient | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 12.4 | — | polycrystal | resistivity | — | 2005 | T2 | cond-mat/0511489 |
| 3.5 | — | polycrystal | resistivity | — | 2004 | T1 | DOI: 10.1103/PhysRevB.70.104520 |
| 3.5 | — | polycrystal | resistivity | — | 2004 | T1 | cond-mat/0403229 |
| — | — | polycrystal | resistivity, susceptibility | — | 2005 | T1 | cond-mat/0502674 |
| — | — | polycrystal | resistivity | — | 2005 | T1 | DOI: 10.1103/PhysRevB.71.134509 |
| — | — | polycrystal | resistivity | — | 2001 | T1 | DOI: 10.1103/PhysRevB.64.094515 |
Structure
- Crystal structure
- tetragonal
- Space group
- I4/mmm
- Phase
- 1222
- Lattice a (Å)
- 3.833
Superconducting parameters
- Pairing symmetry
- d-wave
- λ_eph (e–ph coupling)
- —
Competing orders
- T_AFM
- 180.0 K
Samples & pressure
- Sample form
- polycrystal