Tc max
5.1 K
Tc ambient
5.1 K
arXiv year
2013
Papers
7
Tc exp.
4.8 K
Tc theo.
—
Evidence
experimental
Tc max measured at single_crystal, susceptibility, DOI: 10.1103/PhysRevB.106.054506, confirmed by 3 papers
Evidence (9 records from 7 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 5.1 | — | single_crystal | susceptibility | s-wave | 2022 | T1 | DOI: 10.1103/PhysRevB.106.054506 |
| 5.0 | — | single_crystal | resistivity | s-wave | 2022 | T1 | DOI: 10.1103/PhysRevB.106.054506 |
| 4.8 | — | polycrystal | susceptibility | s-wave | 2014 | T1 | 1406.5627 |
| 4.8 | — | polycrystal | susceptibility | s-wave | 2014 | T1 | DOI: 10.1103/PhysRevB.90.064508 |
| 4.5 | — | single_crystal | susceptibility | s-wave | 2018 | T1 | DOI: 10.1103/PhysRevB.97.024511 |
| 4.5 | ambient | single_crystal | susceptibility, resistivity | — | 2013 | T1 | DOI: 10.1103/PhysRevB.88.020505 |
| 4.5 | — | single_crystal | susceptibility | — | 2013 | T1 | 1305.4109 |
| 4.3 | — | polycrystal | muSR | s-wave | 2014 | T1 | DOI: 10.1103/PhysRevB.90.064508 |
| — | — | single_crystal | susceptibility, neutron | s-wave | 2017 | T1 | 1711.09862 |
Structure
- Crystal structure
- rocksalt
- Space group
- Fm-3m
- Lattice a (Å)
- 6.275
Superconducting parameters
- Pairing symmetry
- s-wave
- Gap structure
- full_gap
- Hc2
- 1.9 T (0 K)
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Sample form
- single_crystal
- Doping type
- hole
- Doping level
- 0.450