Tc max
1.7 K
Tc ambient
—
arXiv year
2010
Papers
3
Tc exp.
1.7 K
Tc theo.
—
Evidence
experimental
Tc max measured at P=7.9 GPa, polycrystal, resistivity, DOI: 10.1103/PhysRevLett.105.157001, confirmed by 3 papers
Evidence (11 records from 3 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 1.7 | 7.9 | polycrystal | resistivity | — | 2010 | T1 | DOI: 10.1103/PhysRevLett.105.157001 |
| 1.7 | 7.9 | — | resistivity | — | 2010 | T1 | 1009.3787 |
| 1.4 | 9.3 | polycrystal | resistivity | — | 2010 | T1 | DOI: 10.1103/PhysRevLett.105.157001 |
| 1.4 | 9.3 | — | resistivity | — | 2010 | T1 | 1009.3787 |
| 1.3 | 5.8 | polycrystal | resistivity | — | 2010 | T1 | DOI: 10.1103/PhysRevLett.105.157001 |
| 1.3 | 5.8 | — | resistivity | — | 2010 | T1 | 1009.3787 |
| 0.8 | 7.9 | — | resistivity | — | 2010 | T1 | 1009.3787 |
| 0.6 | 16.2 | polycrystal | resistivity | — | 2010 | T1 | DOI: 10.1103/PhysRevLett.105.157001 |
| 0.6 | 16.2 | — | resistivity | — | 2010 | T1 | 1009.3787 |
| 0.4 | 16.2 | — | resistivity | — | 2010 | T1 | 1009.3787 |
| 0.1 | 13.5 | single_crystal | resistivity | — | 2020 | T1 | DOI: 10.1103/PhysRevB.101.104501 |
Structure
- Crystal structure
- alpha-PbO
- Space group
- P4/nmm
Superconducting parameters
- Hc2
- 0.6 T (0 K)
- λ_eph (e–ph coupling)
- —