Tc max
0.9 K
Tc ambient
0.9 K
arXiv year
1986
Papers
33
Tc exp.
0.9 K
Tc theo.
—
Evidence
experimental
Tc max measured at polycrystal, susceptibility, DOI: 10.1103/PhysRevB.92.241101, confirmed by 3 papers
Evidence (50 records from 33 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 1.0 | ambient | polycrystal | resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevLett.82.169 |
| 1.0 | ambient | single_crystal | resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevLett.82.169 |
| 0.9 | — | polycrystal | susceptibility | — | 2015 | T1 | DOI: 10.1103/PhysRevB.92.241101 |
| 0.9 | — | thin_film | resistivity | — | 1986 | T1 | DOI: 10.1103/PhysRevB.34.4595 |
| 0.9 | — | polycrystal | susceptibility, resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevB.60.3076 |
| 0.9 | ambient | polycrystal | susceptibility | — | 1992 | T1 | DOI: 10.1103/PhysRevB.45.10544 |
| 0.9 | — | polycrystal | resistivity | — | 2015 | T1 | DOI: 10.1103/PhysRevB.92.241101 |
| 0.9 | — | polycrystal | specific_heat | — | 1991 | T1 | DOI: 10.1103/PhysRevB.44.12074 |
| 0.9 | — | polycrystal | specific_heat | unknown | 2001 | T1 | DOI: 10.1103/PhysRevB.63.100505 |
| 0.9 | — | single_crystal | resistivity | — | 2002 | T1 | DOI: 10.1103/PhysRevLett.88.247005 |
| 0.9 | — | polycrystal | resistivity | unknown | 2000 | T1 | DOI: 10.1103/PhysRevLett.84.5616 |
| 0.9 | ambient | polycrystal | susceptibility | — | 1993 | T1 | DOI: 10.1103/PhysRevB.48.10395 |
| 0.9 | ambient | polycrystal | specific_heat | unknown | 1995 | T1 | DOI: 10.1103/PhysRevB.51.404 |
| 0.9 | — | polycrystal | specific_heat | — | 1986 | T1 | DOI: 10.1103/PhysRevB.33.126 |
| 0.9 | ambient | single_crystal | specific_heat | — | 1998 | T1 | DOI: 10.1103/PhysRevLett.81.4476 |
| 0.9 | — | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.36.2436 |
| 0.9 | ambient | single_crystal | susceptibility | — | 1992 | T1 | DOI: 10.1103/PhysRevB.45.10544 |
| 0.9 | — | polycrystal | specific_heat | — | 1986 | T1 | DOI: 10.1103/PhysRevB.33.3168 |
| 0.9 | — | polycrystal | resistivity | — | 1988 | T1 | DOI: 10.1103/PhysRevB.38.6402 |
| 0.9 | — | single_crystal | specific_heat | unknown | 2015 | T1 | DOI: 10.1103/PhysRevLett.114.147002 |
| 0.9 | — | polycrystal | resistivity | — | 1986 | T1 | DOI: 10.1103/PhysRevLett.57.238 |
| 0.9 | — | single_crystal | susceptibility | p-wave | 1986 | T1 | DOI: 10.1103/PhysRevLett.56.2513 |
| 0.9 | — | polycrystal | susceptibility, muSR | — | 1986 | T1 | DOI: 10.1103/PhysRevLett.57.1255 |
| 0.8 | ambient | polycrystal | resistivity, specific_heat, susceptibility | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| 0.8 | — | single_crystal | susceptibility, neutron | unknown | 2014 | T1 | DOI: 10.1103/PhysRevB.89.235118 |
| 0.8 | — | single_crystal | muSR | — | 2000 | T1 | DOI: 10.1103/PhysRevB.61.6377 |
| 0.8 | — | single_crystal | specific_heat | — | 2016 | T1 | DOI: 10.1103/PhysRevB.93.024502 |
| 0.8 | — | polycrystal | specific_heat | — | 2003 | T2 | cond-mat/0306451 |
| 0.8 | — | polycrystal | specific_heat | unknown | 1999 | T1 | cond-mat/9912398 |
| 0.8 | — | polycrystal | specific_heat | — | 2003 | T2 | cond-mat/0306451 |
| — | 0.7 | polycrystal | specific_heat | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 1.2 | polycrystal | specific_heat | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 2.9 | polycrystal | specific_heat | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 2.1 | polycrystal | resistivity | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 2.8 | polycrystal | resistivity | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 3.6 | polycrystal | resistivity | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 4.3 | polycrystal | resistivity | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 5.6 | polycrystal | resistivity | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | 5.9 | polycrystal | resistivity | p-wave | 2019 | T1 | DOI: 10.1103/PhysRevLett.122.067001 |
| — | — | — | heat_capacity, susceptibility | — | 2002 | T1 | cond-mat/0207442 |
| — | — | — | — | — | 2001 | T1 | cond-mat/0104445 |
| — | — | polycrystal | STM | unknown | 2000 | T2 | cond-mat/0008342 |
| — | 0.4 | polycrystal | resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevLett.82.169 |
| — | 0.6 | polycrystal | resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevLett.82.169 |
| — | 1.0 | polycrystal | resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevLett.82.169 |
| — | 2.0 | polycrystal | resistivity | — | 1999 | T1 | DOI: 10.1103/PhysRevLett.82.169 |
| — | — | single_crystal | susceptibility | — | 1998 | T1 | DOI: 10.1103/PhysRevB.57.3640 |
| — | — | polycrystal | muSR | unknown | 1989 | T1 | DOI: 10.1103/PhysRevB.39.11345 |
| — | — | single_crystal | neutron | — | 1986 | T1 | DOI: 10.1103/PhysRevB.34.4382 |
| — | — | — | — | — | 1986 | T1 | DOI: 10.1103/PhysRevB.34.6546 |
Structure
- Crystal structure
- cubic
- Space group
- Fm3c
Superconducting parameters
- Pairing symmetry
- p-wave
- λ_eph (e–ph coupling)
- 0.04
Competing orders
- ρ(T) exponent
- 1.00
Samples & pressure
- Sample form
- polycrystal
- Substrate
- sapphire