Tc max
92.0 K
Tc ambient
92.0 K
arXiv year
1987
Papers
8
Tc exp.
92.0 K
Tc theo.
—
Evidence
experimental
Tc max measured at ambient, polycrystal, susceptibility, DOI: 10.1103/PhysRevB.35.7119, confirmed by 3 papers
Evidence (13 records from 8 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 94.5 | ambient | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.7119 |
| 92.0 | ambient | polycrystal | susceptibility | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.7119 |
| 92.0 | — | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.8767 |
| 92.0 | — | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.36.8819 |
| 91.2 | ambient | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.7119 |
| 90.0 | — | — | resistivity | — | 2017 | — | 1703.08707 |
| 90.0 | ambient | polycrystal | — | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.8709 |
| 90.0 | ambient | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.36.843 |
| 90.0 | — | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.8767 |
| 90.0 | ambient | polycrystal | resistivity | — | 1987 | T1 | DOI: 10.1103/PhysRevB.36.743 |
| 85.0 | ambient | polycrystal | susceptibility | — | 1987 | T1 | DOI: 10.1103/PhysRevB.35.8791 |
| 80.0 | — | — | resistivity | — | 2017 | — | 1703.08707 |
| 54.0 | ambient | polycrystal | resistivity, susceptibility | — | 1987 | T1 | DOI: 10.1103/PhysRevB.36.743 |
Superconducting parameters
- Pairing symmetry
- d-wave
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Sample form
- polycrystal
- Pressure type
- none