Tc max
87.0 K
Tc ambient
87.0 K
arXiv year
1989
Papers
8
Tc exp.
86.5 K
Tc theo.
—
Evidence
experimental
Tc max measured at single_crystal, susceptibility, DOI: 10.1103/PhysRevB.76.144505, confirmed by 2 papers
Evidence (12 records from 8 papers)
the flat columns above are aggregates — each line here is one paper's claim| Tc (K) | P (GPa) | Sample | Method | Pairing | Year | Tier | Paper |
|---|---|---|---|---|---|---|---|
| 87.0 | — | single_crystal | susceptibility | d-wave | 2007 | T1 | DOI: 10.1103/PhysRevB.76.144505 |
| 86.5 | — | polycrystal | susceptibility | — | 1989 | T1 | DOI: 10.1103/PhysRevB.39.9192 |
| 79.5 | — | polycrystal | susceptibility | — | 1989 | T1 | DOI: 10.1103/PhysRevB.39.9192 |
| 79.0 | — | thin_film | susceptibility | d-wave | 1996 | T1 | DOI: 10.1103/PhysRevB.53.11352 |
| 78.0 | — | single_crystal | susceptibility | d-wave | 2007 | T1 | DOI: 10.1103/PhysRevB.76.144505 |
| 71.0 | ambient | thin_film | susceptibility | — | 1993 | T1 | DOI: 10.1103/PhysRevB.47.11439 |
| 70.0 | — | thin_film | susceptibility | d-wave | 1996 | T1 | DOI: 10.1103/PhysRevB.53.11352 |
| 70.0 | — | thin_film | susceptibility | — | 1994 | T1 | DOI: 10.1103/PhysRevB.49.15970 |
| 68.0 | — | thin_film | susceptibility | d-wave | 1996 | T1 | DOI: 10.1103/PhysRevB.53.11352 |
| — | — | powder | susceptibility | — | 2013 | T1 | 1302.6877 |
| — | — | single_crystal | resistivity | — | 1996 | T1 | DOI: 10.1103/PhysRevB.53.5922 |
| — | — | single_crystal | resistivity | — | 1996 | T1 | DOI: 10.1103/PhysRevB.54.6785 |
Structure
- Crystal structure
- orthorhombic
- Phase
- cuprate_123
- Lattice a (Å)
- 3.817
- Lattice c (Å)
- 11.674
Superconducting parameters
- Pairing symmetry
- d-wave
- Gap structure
- nodal
- λ_eph (e–ph coupling)
- —
Samples & pressure
- Substrate
- SrTiO3
- Doping type
- isovalent
- Doping level
- 0.030